A satin varnish like TotalBoat Halcyon Water-Based Marine Varnish, a matte varnish like TotalBoat Lust Rapid Recoat Marine Spar Varnish, or another epoxy-compatible finish can be applied.
Epoxy substrates need to cure for at least 5-7 days prior to any surface preparation or applying other coatings. Once cured, the epoxy must be washed with a mild soap and warm water, then rinsed well to remove any possible amine blush, whether noticeable or not. This must be performed even if the epoxy is considered non-blushing or does not appear to have an amine blush on the surface.
Dry the surface completely. Sand the surface with 220-grit or 320-grit sandpaper. A DA (dual-action) sander can help reduce a sense of grain or sanding marks that show a sense of sanding direction. Remove any sanding residue by wiping the surface clean with a clean, lint-free cotton rag wetted with one of the specified cleaner/surface preparation solvents, and allow the surface to dry completely.